2024年7月9日星期二

Induction Brazing Carbide

Induction Brazing Carbide File Objective: Induction Brazing carbide rotary file assemblies with uniform concentricity in an aerospace application Material • Carbide blank • High speed steel shank • Temperature indicating paint • Braze shim and black flux Temperature 1400°F (760°C) Frequency 550 kHz Equipment: DW-UHF-4.5kw induction heating system, equipped with a remote heat station containing two 0.33 μF capacitors (total 0.66 μF) An induction heating coil designed and developed specifically for this application. Process A multi-turn helical coil is used. The part is heated to determine the time required to reach the desired temperature and required heat pattern. It takes approximately 30 - 45 seconds to reach 1400°F (760°C) depending on the various part sizes. Flux is applied to the entire part. A braze shim is sandwiched between the steel shank and carbide. Induction heating power is applied until the braze flows. With proper fixturing, concentricity of the part can be achieved. Results/Benefits • Repeatable, consistent precise heat.   https://dw-inductionheater.com/induction-brazing-carbide-file.html?feed_id=253337&_unique_id=668d6f6a2c054

2024年7月2日星期二

Brazing carbide shaft with induction

Brazing carbide shaft with induction Objective: Braze a carbide shaft to a steel tube Material: Carbide shaft 1/8" to 1" diameter (varying sizes) Steel tube 3/8" to 1 ¼" OD Silver solder braze Temperature: indicating paint Temperature: 1400 °F for 60 seconds Frequency300 kHz Equipment: DW-UHF-6KW-III, 150-400 kHz solid state induction heating system equipped with a remote heat station containing two 0.66 μF capacitors (total 1.32 μF) A multi-turn helical coil Process: Silver solder is applied to where the carbide shaft and steel tube meet. The clearance between the two parts is approximately .0005". A small piece of solder braze is placed on the part and then the part is heated. It takes about 60 seconds to flow the braze with the best heat migration and solder flow. Even though the part can be heated faster, optimal results are obtained at 60 seconds. Results/Benefits: Induction heating provides even, precise heat. Precise directed heat is required for the solder braze to flow evenly around the part to assure a good joint. https://dw-inductionheater.com/brazing-carbide-shaft-with-induction.html?feed_id=252358&_unique_id=6684270e9841c

2024年6月26日星期三

Brazing Carbide To Steel With Induction

Brazing Carbide To Steel With Induction  Objective: Braze carbide rotary file assemblies with uniform concentricity in an aerospace application Material : • Carbide blank • High speed steel shank • Temperature indicating paint • Braze shim and black flux Temperature 1400°F (760°C) Frequency 252 kHz Equipment DW-UHF-10kw induction heating system, equipped with a remote heat station containing two 0.33 μF capacitors (total 0.66 μF) An induction heating coil designed and developed specifically for this application. Process A multi-turn helical coil is used. The part is heated to determine the time required to reach the desired temperature and required heat pattern. It takes approximately 30 - 45 seconds to reach 1400°F (760°C) depending on the various part sizes. Flux is applied to the entire part. A braze shim is sandwiched between the steel shank and carbide. Induction heating power is applied until the braze flows. With proper fixturing, concentricity of the part can be achieved. Results/Benefits • Repeatable, consistent precise heat. https://dw-inductionheater.com/brazing-carbide-to-steel-with-induction.html?feed_id=251678&_unique_id=667d02fb8f6ce

2024年6月25日星期二

Brazing Carbide Tool Tips With Induction

Brazing Carbide Tool Tips With Induction  Objective: Attaching carbide cutters to a steel meat cutter impeller Material carbide blocks; steel shank fitting Temperature 1400 °F (760 °C) Frequency 300 kHz Equipment DW-UHF-30KW induction heating systems including: Induction heating coil Workhead: two-cap 1.0μF (Total 0.5 μF) Process The entire part is placed in a five-turn helical coil, the power is applied until the part is heated to the required temperature and a uniform heat pattern is achieved. The coil allows for easy fixturing and uniformity of heating between the carbide and the steel shank for a premium braze joint. Results/Benefits Precision: Due to the size of the induction coil, the process allows for precise placement of the carbides on the steel shanks Economy: Power is consumed only during the heat cycle Repeatability: joint quality is maintained in this repeatable process https://dw-inductionheater.com/brazing-carbide-tool-tips-with-induction.html?feed_id=251542&_unique_id=667b95093f9fb

2024年6月20日星期四

Brazing Carbide To Steel Shank

Brazing Carbide To Steel Shank with Induction Objective :Brazing carbide teeth to a steel jaw in less than 5 minutes Material: Steel pipe jaw, 0.5” (12.7mm) dia, 1.25” (31.75mm) long, 0.25”(6.35mm) thick carbide teeth, black flux and silver copper braze shims Temperature: 1292ºF (700ºC) Frequency: 300kHz Equipment • DW-UHF-10kW induction heating system, equipped with a remote workhead containing one 0.66μF capacitor • An induction heating coil designed and developed specifically for this application. Process: A two turn rectangular helical coil is used to heat the carbide and steel to 1292ºF (700ºC) for 4 to 5 minutes. Three braze shims control the amount of braze and the even heat allows for a good flow of braze creating an aesthetically pleasing bond. Results/Benefits Induction heating provides: • Hands-free heating that involves no operator skill for manufacturing • Consistent, repeatable aesthetically pleasing brazes • Even distribution of heating https://dw-inductionheater.com/brazing-carbide-to-steel-shank.html?feed_id=250672&_unique_id=6674711612cba

2024年6月13日星期四

Induction Brazing Steel To Carbide Plate

Induction Brazing Steel To Carbide Plate Objective Brazing a steel piston valve assembly Material Steel piston valve 4.5” dia (11.43cm), tungsten carbide plate and braze Temperature 1350 ºF Frequency 100 kHz Equipment •DW-UHF-40kW induction heating system, equipped with a remote workhead containing six 1.0μF capacitors for a total of 1.5μF • An induction heating coil designed and developed specifically for this application. Process A five turn pancake coil is used to braze the piston valve and tungsten carbide plate. The assembly was heated for 10 minutes to flow the braze and join the two pieces. Results/Benefits Induction heating provides: • Rapid localized heat, which can minimize oxidation and reduce cleaning after joining • Hands-free heating that involves no operator skill for manufacturing • Clean and controllable joints • Produces high quality repeatable parts https://dw-inductionheater.com/induction-brazing-steel-to-carbide.html?feed_id=249813&_unique_id=666bdf20c06c2

2020年5月18日星期一

induction brazing steel carbide cap to shaft




Objective

High Frequency Induction brazing steel carbide cap to shaft.  Customer currently uses a torch process, but would like to change to induction brazing in order to reduce scrap and rework and improve the quality of the braze.





Equipment

DW-UHF-6kw-III handheld induction brazing heater


handheld inductino heater


Materials

• Carbon steel

• magnetic carbide caps

• Alloy – EZ Flo 3 paste

• Test 1: Shaft Diameter: 0.5” (12.7 mm)

• Test 2: Shaft Diameter: 0.375” (9.525mm)

• Test 3: Shaft Diameter: 0.312” (7.925mm)









Key Parameters

Test 1: Shaft Diameter: 0.5” (12.7mm)

Temperature: Approximately 1450°F (788°C)

Power: Pre-curie – 3.3 kW

Time: 11 seconds









Key Parameters

Test 2: Shaft Diameter: 0.375” (9.525mm)

Temperature: Approximately 1450°F (788°C)

Power: Pre-curie – 1.8 kW

Time: 8 seconds









Key Parameters

Test 3: Shaft Diameter: 0.312” (7.925mm)

Temperature: Approximately 1450°F (788°C)

Power: Pre-curie – 1.7 kW

Time: 7.5 seconds









Process:



  1. Paste alloy was applied to the cone shape top of each steel shaft.

  2. The cap was set on top and rotated to distribute the paste alloy.

  3. Each assembly was positioned in the coil and heated.

  4. Preliminary heat tests were conducted using tempilaq paint to estimate the heat cycle to 1450 degrees F.


Results/Benefits:



  • Precise control of the time and temperature resulting in improved quality and consistent result

  • Power on demand with rapid heat cycles

  • Repeatable process, not operator dependent

  • Safe induction heating with no open flames

  • Energy efficient heating







https://dw-inductionheater.com/wp-content/uploads/2020/05/induction-brazing-steel-carbide-cap.png?v=1589810073
https://dw-inductionheater.com/induction-brazing-steel-carbide-cap-to-shaft.html
brazing carbide joints, brazing steel carbide, HF brazing carbide process, HF brazing steel carbide system, high frequency brazing carbide system, induction brazing carbide, induction brazing carbide machine, induction brazing steel, induction brazing steel machine, steel carbide

2020年4月22日星期三

Induction Brazing Carbide To Steel






Objective

Induction Brazing carbide to steel parts



Equipment

DW-HF-15kw Induction Heating Power Supply


HLQ custom coil


Key Parameters

Power: 5.88 kW

Temperature: Approximately 1500°F (815°C)

Time: 10 sec



Materials

Coil- 

2 helical turns (20 mm ID)

1 planar turn (40 mm OD, 13 mm Height)



Carbide- 

13 mm OD, 3 mm wall thickness


Steel piece–

20 mm OD, 13 mm ID













Process:



  1. To demonstrate elimination of “hand feeding” the alloy, we formed the alloy into a ring to tightly fit over the center post tube. This method provides a uniform amount for each cycle, resulting in uniform joints and wetting.

  2. The custom made coil was then placed over the steel piece, where is was set for 10 seconds to heat the alloy.

  3. The alloy was heated at approximately 1500°F (815)°C

  4.  The whole piece is left alone and cooled with ambient air




Results/Benefits:



  • Induction Brazing was successful all in under 15 seconds with 8kW

  • High quality and repeatability of the brazed joints

  • Increased productivity

  • Rings will need to be developed for specific joints to prevent the use of too much alloy

  • Precise control of the time and temperature









https://dw-inductionheater.com/wp-content/uploads/2020/04/induction-brazing-carbide-to-steel-part-process-1024x819.png
https://dw-inductionheater.com/induction-brazing-carbide-to-steel-parts.html
brazing carbide, brazing carbide machine, Brazing carbide to steel, carbide to steel brazing, HF brazing carbide, high frequency brazing carbide, induction brazing carbide, Induction Brazing Carbide to Steel, induction soldering carbide, radio frequency brazing carbide, soldering carbide to steel

2020年3月28日星期六

Induction Brazing Steel Parts to Tungsten Carbide Plate

Induction Brazing Steel Parts to Tungsten Carbide Plate


Objective

Induction Brazing of Steel Parts to a Tungsten Carbide Plate


Equipment


DW-UHF-6KW-III handheld induction brazing machine


Induction brazing steel parts







Test 1


Materials
• Steel rod: 19.05 mm (0.75″) OD, 82.55 mm (3.25″) Length


• Tungsten Carbide Plate: 38.1 mm (1.5″) OD, 10.16 mm (0.4″) Thickness


• Alloy: 19.05 mm (0.75″) Brazing discs


Power: 4.0 kW
Temperature: Approximately 760° C (1400° F)
Time: 40 sec









Test 2


Materials
• Steel rod: 12.7 mm (0.50″) OD, 76.2 mm (3″) Length


• Tungsten Carbide Plate: 19.05 mm (0.75″) OD, 6.35 mm (0.25″) Thickness


• Alloy: 12.7 mm (0.50″) Brazing discs


Power: 2.36 kW
Temperature: Approximately 760° C (1400° F)
Time: 23 sec









Test 3


Materials
• Steel rod: 12.7 mm (0.50″) OD, 76.2 mm (3″) Length


• Tungsten Carbide Plate: 1″ OD, 1.39mm (0.055″) Thickness


• Alloy: 12.7 mm (0.50″) Brazing discs


Power: 2.36 kW
Temperature: Approximately 760° C (1400° F)
Time: 20-25 sec (Pulsing on/off)









Test 4


Materials
• Steel rod: 6.35 mm (0.25″) OD, 76.2 mm (3″) Length


• Tungsten Carbide Plate: 21.08mm (0.83″) OD, 1.65mm (0.065″) thicknes


• Alloy: 6.35 mm (0.25″) Brazing discs


Power: 1.96 kW
Temperature: Approximately 760° C (1400° F)Induction brazing steel carbideInduction brazing steel partsInduction brazing steel parts
Time: 20 sec (Pulsing on/off)













Results and Conclusions:


Brazing of different steel parts to carbide disks is possible with one induction coil. Power was regulated by turning the heat on and off using a foot switch to prevent overheating of the carbide parts.







 













https://dw-inductionheater.com/wp-content/uploads/2020/03/4C736463-2605-4E33-8201-8092BCECA194-1024x633.jpeg
https://dw-inductionheater.com/induction-brazing-steel-parts-to-tungsten-carbide-plate.html
brazing carbide, brazing steel, brazing steel parts, Brazing tungsten carbide, High Frequency Brazing steel, induction brazing carbide, induction brazing steel, steel brazing

关注者

我的简介

我的照片
HLQ induction heating machine manufacturer provides the service of induction brazing,melting,hot forming,hardening surface,annealing,shrink fitting,PWHT,etc.