Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
https://dw-inductionheater.com/induction-annealing-aluminum-pipe.html?feed_id=229116&_unique_id=652d609008891
2023年10月16日星期一
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
https://dw-inductionheater.com/induction-annealing-aluminum-pipe.html?feed_id=229116&_unique_id=652d609008891
2023年7月20日星期四
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2023年4月16日星期日
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2023年4月10日星期一
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2022年12月28日星期三
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2022年10月9日星期日
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2022年9月25日星期日
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2022年9月12日星期一
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2022年6月24日星期五
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2022年6月3日星期五
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2022年4月14日星期四
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
2022年3月1日星期二
Induction Annealing Aluminum PIpe
Induction Annealing Aluminum PIpe With High Frequency Induction Heating Machine
Objective Annealing aluminum fuel tank fill neck to 650 ºF (343 ºC)
Material Aluminum fill neck 2.5” (63.5mm) diameter, 14” (35.5cm) long
Temperature 650 ºF (343 ºC)
Frequency 75 kHz
Equipment •DW-HF-45kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF
• An induction heating coil designed and developed specifically for this application.
Process An eight turn helical is used to heat the tube for annealing. To anneal the full length of the tube, the tube is placed in the coil and heated for 30 seconds then rotated and the bottom half is heated for an additional 30. The tube is then bent while hot to prevent cracking.
Results/Benefits Induction heating provides:
• High efficiency, low energy cost
• Fast, controllable and repeatable process
• Prevention of cracks
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
订阅:
博文 (Atom)
关注者
我的简介
- HLQ induction heating machine
- HLQ induction heating machine manufacturer provides the service of induction brazing,melting,hot forming,hardening surface,annealing,shrink fitting,PWHT,etc.